Home » Calculators » Wet Processing » Wet Processing (Dyeing & Printing) » Mercerisation Baume, NaOH Concentration & Barium Activity Number
Jump to a calculator 618 tools

Preparation

Mercerisation Baume, NaOH Concentration & Barium Activity Number

Put this calculator on your own site

Paste this where you want the calculator to appear. It works on any site — WordPress, Squarespace, Webflow, Ghost or plain HTML — and needs no JavaScript of yours. It carries a link back here, which is the only thing we ask for it.

See what it looks like

The hydrometer measures the tank. Only the barium activity number measures the cotton.

Liquor Strength What the hydrometer reads, and what the goods carry away
deg Be

Full mercerising is normally 28-32 deg Be

kg
%
Barium Activity (AATCC 89) Millilitres of acid to titrate the residual barium hydroxide
mL

Barium hydroxide with no specimen

mL
mL

Sodium Hydroxide

— % w/w

From the Baume reading, through specific gravity

Liquor, Charge & Degree of Mercerisation

Specific Gravity
—
Sodium Hydroxide
— g/L
Caustic Carried on the Goods
— kg
Barium Activity Number
—
Barium Uptake vs Unmercerised
— x
Strength vs Full-Mercerising Threshold
— %

The per cent NaOH fit is valid from 8 to 32% w/w, which is roughly 11 to 36 degrees Baume, and covers slack through full mercerising; do not extrapolate it to caustic recovery liquors or to the dilute alkali of a scouring bath. Baume readings must be temperature-corrected to the scale reference before conversion - the scale is defined at 60 F and a tank run at 20 C or higher reads low, which understates the true concentration. The barium activity number is a relative measure that depends on the unmercerised control being genuinely comparable cotton; a control of different origin, maturity or preparation history moves the denominator and with it the reported result. Barium activity also cannot distinguish tension-mercerised from slack-mercerised goods, because both convert the lattice - lustre has to be assessed separately.

Using this calculator

About the Mercerisation Baume, NaOH Concentration & Barium Activity Number

The formula

This is the expression the tool evaluates. Every term is named underneath, with the unit it must be supplied in.

Baume to specific gravity, heavy-liquid scale
specificGravity = 145 / ( 145 - baume )

Baume is a hydrometer scale, not a concentration. The heavy-liquid form applies to anything denser than water, which caustic soda is. Note that some older references use 144.3 rather than 145 as the modulus; the difference reaches about 0.15% in specific gravity over the mercerising range.

Specific gravity to per cent NaOH
naohPercent = 8 + ( specificGravity - 1.0869 ) x 91.57

Sodium hydroxide solutions are close to linear in density against concentration between 8 and 32% w/w, which covers every mercerising liquor. This fit reproduces the published density table to within 0.1 percentage points across that band. Outside it the relationship curves and this expression should not be used.

Per cent by weight to grams per litre
naohGramsPerLitre = specificGravity x 1000 x naohPercent / 100

Per cent is a mass fraction and grams per litre is a mass concentration; the density is what converts between them. A litre of 30 deg Be liquor weighs 1.26 kg, so 23.9% of it is 302 g of caustic and not 239 g.

AATCC 89 barium activity number
bariumActivityNumber = 100 x ( blankTitre - sampleTitre ) / ( blankTitre - controlTitre )

Mercerised cellulose adsorbs more barium hydroxide than unmercerised cellulose, so less remains in solution and less acid is needed to titrate it. Each difference from the blank is the barium the specimen took up, and the ratio of the two uptakes, scaled by 100, is the activity number.

Symbols used above
SymbolStands forUnit
deg BeDegrees Baume, hydrometer scale for liquids denser than water—
SGSpecific gravity, density relative to water—
BANBarium activity number; unmercerised cotton is 100 by definition—
WPUWet pickup, liquor retained as a percentage of dry fabric mass%

How the result is derived

Step by step, from the values you type to the figure on screen.

  1. The 6 inputs are read from the form on every keystroke: Liquor Strength, Fabric Through the Range, Wet Pickup, Blank Titre, Unmercerised Control Titre and Mercerised Sample Titre.
  2. Each value is checked against the accepted range in the input table below. A value outside its range stops the calculation rather than producing a misleading figure — the results blank out and a message appears.
  3. The validated values are substituted into the expression above, which resolves Sodium Hydroxide together with every supporting figure in one pass — no value is carried over from a previous entry.
  4. The supporting outputs — Specific Gravity, Sodium Hydroxide, Caustic Carried on the Goods, Barium Activity Number, Barium Uptake vs Unmercerised and Strength vs Full-Mercerising Threshold — come from the same pass, so they always describe the same case as the headline figure.
  5. Results are rounded for display only. The full-precision value is used throughout the chain, so reading a rounded intermediate figure back into the tool by hand can shift the last digit.

What each input means

Where to read each value on the floor, the unit it must be in, and the range the tool accepts.

InputUnitAccepted rangeDefaultWhat it means
Liquor Strengthdeg Be8 to 40 deg Be30Full mercerising is normally 28-32 deg Be
Fabric Through the Rangekg1 to 20000 kg500
Wet Pickup%30 to 200 %85
Blank TitremL5 to 100 mL42.5Barium hydroxide with no specimen
Unmercerised Control TitremL1 to 100 mL36
Mercerised Sample TitremL1 to 100 mL33.4

What the tool returns

The headline figure and every supporting value it is built from.

OutputUnitWhat it tells you
Sodium Hydroxide (headline result)% w/wFrom the Baume reading, through specific gravity
Specific Gravity—
Sodium Hydroxideg/L
Caustic Carried on the Goodskg
Barium Activity Number—
Barium Uptake vs Unmercerisedx
Strength vs Full-Mercerising Threshold%

Worked example

Given

0
Liquor at 30 deg Be
1
500 kg of fabric through the range at 85% wet pickup
2
Titres: blank 42.5 mL, unmercerised control 36.0 mL, mercerised sample 33.4 mL

Substituting

SG = 145 / (145 - 30) = 145 / 115 = 1.26087NaOH% = 8 + (1.26087 - 1.0869) x 91.57 = 8 + 15.93 = 23.93%g/L = 1.26087 x 1000 x 0.2393 = 301.7Carried caustic = 500 x 0.85 x 301.7 / 1000 = 128.2 kgBAN = 100 x (42.5 - 33.4) / (42.5 - 36.0) = 100 x 9.1 / 6.5 = 140

Answer

0
Specific gravity 1.2609, sodium hydroxide 23.93% w/w
1
301.7 g/L in the tank
2
128.2 kg of caustic carried away on the goods
3
Barium activity number 140 - fully mercerised
4
Liquor is at 116% of the full-mercerising threshold

The 128 kg of caustic riding out of the mangle on half a tonne of cloth is the number that pays for a caustic recovery plant. It is not consumed by the reaction - almost all of it is recoverable by evaporation, and it is the single largest chemical stream in a mercerising range.

How to use it

  1. Work through the input groups in order — Liquor Strength and Barium Activity (AATCC 89). The defaults are a realistic case, so you can change one value at a time and watch what moves.
  2. There is no calculate button. Every figure recalculates as you type or drag, which is what makes this usable for a what-if sweep rather than a single answer.
  3. Read Sodium Hydroxide in the dark results panel — that is the headline figure, expressed in % w/w.
  4. Check the supporting rows underneath (Specific Gravity, Sodium Hydroxide, Caustic Carried on the Goods, Barium Activity Number, Barium Uptake vs Unmercerised and Strength vs Full-Mercerising Threshold) before acting on the headline — they are where an implausible input usually shows itself first.
  5. Reset to defaults returns every field to the reference case, which is the quickest way to check whether a surprising result came from the tool or from an input you had changed earlier.

Where this is used

  • Process planning — establishing Sodium Hydroxide before a trial is booked, so machine time and material in Wet Processing (Dyeing & Printing) are committed against a calculated figure rather than an estimate.
  • Costing and quotation — Sodium Hydroxide is an input to the cost sheet, and quoting from a worked number rather than a remembered one is what keeps a margin intact.
  • Troubleshooting — when the floor result drifts from plan, entering the measured values (starting with Liquor Strength) shows how much of the gap in Sodium Hydroxide each variable explains.
  • Teaching and study — the accepted ranges bracket normal Wet Processing (Dyeing & Printing) practice, so moving one variable at a time shows the shape of the relationship rather than a single answer.

Reading the result

Typical bands and what each one is telling you.

ValueWhat it indicates
BAN 100Unmercerised cotton, by definition of the test.
BAN 105 - 115Slack or partial mercerisation. Lustre gain is marginal.
BAN 130 - 150Full commercial mercerisation. Dye uptake, lustre and strength all improved.
24 - 32 deg BeWorking range for full mercerising, roughly 240 to 330 g/L NaOH.
below 18 deg BeBelow the swelling threshold. The cotton swells but the lattice does not convert.

Assumptions and limits

  • The per cent NaOH fit is valid from 8 to 32% w/w, which is roughly 11 to 36 degrees Baume, and covers slack through full mercerising; do not extrapolate it to caustic recovery liquors or to the dilute alkali of a scouring bath. Baume readings must be temperature-corrected to the scale reference before conversion - the scale is defined at 60 F and a tank run at 20 C or higher reads low, which understates the true concentration. The barium activity number is a relative measure that depends on the unmercerised control being genuinely comparable cotton; a control of different origin, maturity or preparation history moves the denominator and with it the reported result. Barium activity also cannot distinguish tension-mercerised from slack-mercerised goods, because both convert the lattice - lustre has to be assessed separately.
  • Every input is bounded to the range normal practice occupies (Liquor Strength 8 to 40 deg Be, Fabric Through the Range 1 to 20000 kg and Wet Pickup 30 to 200 %, and so on for the rest). Those bounds are guard rails against typing errors, not a claim that the formula fails one unit outside them.
  • The calculation is deterministic: the same inputs always give the same result. It carries no allowance for machine condition, operator skill, ambient conditions or lot-to-lot material variation unless an input above explicitly represents one.
  • Nothing is sent anywhere. The maths runs in your browser, so the numbers you type never leave the page.

Standards and further reading

  • AATCC Test Method 89 - Mercerization in Cotton, which defines the barium activity number and the titration this tool computes it from.
  • ASTM D629 - Quantitative Analysis of Textiles, for the associated compositional work.
  • ISO 105-A01 - preparation of specimens, used when the mercerised goods go on to fastness testing.
  • Baume scale, heavy form: SG = 145 / (145 - deg Be), the National Bureau of Standards convention at 60 F.

On this site

Articles that explain what this tool calculates.

Questions people ask

Why is Baume still used when specific gravity is what the equation needs?

Because a Baume hydrometer is a stick that floats in the tank and can be read by eye from the walkway, at temperature, without sampling anything. It is a shop-floor instrument with a century of habit behind it. The conversion is exact arithmetic, so nothing is lost - but the reading must be temperature-corrected, since a hot liquor is less dense and reads low, and a mercerising tank is rarely at the 60 F the scale is defined for.

Can a high caustic concentration alone guarantee good mercerisation?

No, and this is why the barium activity number exists. Concentration sets whether the cellulose I lattice can convert to cellulose II at all - below about 18 deg Be it cannot, whatever else is done. Above that, the result also depends on temperature, dwell time, tension and how well the liquor penetrates. A tank at 30 deg Be running too fast, too hot, or on inadequately prepared cloth will produce a barium activity number in the 110s. Only the test on the fabric closes the loop.

Why does mercerising need tension, and does this tool account for it?

Caustic swells cotton and the fibre tries to contract; held under tension while it is washed off, the swollen fibre is fixed in a rounder, smoother cross-section that reflects light, which is the lustre. Released without tension it gives slack mercerisation - improved dye uptake and strength but no lustre. This tool computes liquor chemistry and the barium result, both of which are tension-independent; the lustre outcome is not calculated here because it depends on the mechanical arrangement of the range.

What is the caustic carried on the goods figure for?

Two things. It sizes the caustic recovery plant, because that mass leaves the mercerising tank on the cloth and arrives in the wash boxes as weak lye to be evaporated back to strength. And it sizes the neutralisation demand: whatever is not recovered has to be washed out and neutralised with acid, and it is the dominant load on the effluent pH from a mercerising range.

Scroll to Top

Follow on WhatsApp

Scan with your phone’s camera to open the channel, then tap Follow.

QR code for the WhatsApp channelOr open WhatsApp on this device