Synthetic fibres are man-made fibres spun from polymers that are themselves made in a chemical plant, almost all of them from oil and natural gas. The main examples are polyester, nylon (polyamide), polypropylene, acrylic and elastane (spandex). They are one branch of the man-made fibres: the other main branch, the regenerated fibres such as viscose rayon, lyocell and acetate, is made from the natural cellulose of wood pulp, and a third, the inorganic fibres, includes glass and carbon. Synthetic fibres are strong, light, quick-drying and absorb little water, and most of them melt when heated. They are also most of the fibre the world makes: about 91 million tonnes in 2024, 69% of all fibre, with polyester alone at 59% (Textile Exchange, Materials Market Report 2025).
Below, the short answers come first: what the words mean, the examples, and whether a given fibre is synthetic. Then how synthetic fibres are made, a property table against cotton, viscose and wool, how to tell them apart, their uses, how much is made, and what they do to the environment. Three of the site’s calculators are worked through, each with a link that opens the tool with the same figures entered. Each fibre has its own page on this site, linked where it comes up.
Last verified: 18 November 2026. Sources are linked where they are used and listed at the end.
What are synthetic fibres?
A synthetic fibre is a fibre whose polymer does not exist in nature. Chemists build it from small molecules, called monomers, which are joined into long chains (polymerisation); the polymer is then melted or dissolved and forced through the fine holes of a spinneret to form filaments. The US Environmental Protection Agency’s description of the industry puts it in one line: “True synthetics are products of the polymerization of smaller chemical units into long-chain molecular polymers”, while the semisynthetics “are formed from natural polymeric materials such as cellulose” (US EPA, AP-42 section 6.9, Synthetic Fibers).
Labelling law defines each fibre by that chemistry. US law first separates natural from manufactured fibres: a manufactured fibre is “any fiber derived by a process of manufacture from any substance which, at any point in the manufacturing process, is not a fiber” (15 U.S.C. 70(d)). The Federal Trade Commission’s list of generic names then defines most synthetics in the same words, “a manufactured fiber in which the fiber-forming substance is any long chain synthetic polymer”, followed by the chemistry that makes it polyester, acrylic, olefin or spandex (16 CFR 303.7). The EU’s textile regulation lists the fibre names that may appear on a label and defines each one (Regulation (EU) No 1007/2011, Annex I), and the international list of man-made fibre names is ISO 2076.
“Synthetic” is a description, not a label name. A care label names the fibre itself, such as polyester or elastane, never “synthetic”.
Synthetic, man-made, artificial: what the words mean
The three words are often used as if they meant the same thing, and in everyday English they nearly do. In the textile trade they are used more carefully:
| Term | What it covers | Examples |
|---|---|---|
| Man-made, manufactured or artificial fibres | Every fibre made by a manufacturing process, whatever the raw material | All the fibres in the three rows below |
| Synthetic fibres | Man-made fibres from polymers made by chemical synthesis, mostly from oil and gas | Polyester, nylon, polypropylene, acrylic, elastane, aramid |
| Regenerated or semi-synthetic fibres | Man-made fibres from a natural polymer, usually cellulose from wood, dissolved and re-formed | Viscose (rayon), modal, lyocell, cupro, acetate |
| Inorganic man-made fibres | Fibres drawn from minerals, or carbonised | Glass, basalt, carbon, ceramic and metal fibres |
So every synthetic fibre is man-made, but not every man-made fibre is synthetic. Viscose rayon is the commonest example of a man-made fibre that is not synthetic, and it behaves much more like cotton than like polyester: it absorbs water and burns like paper. The classification tree on the fibre-list page places every fibre, natural and man-made.
Examples of synthetic fibres
Five fibres make up almost all synthetic fibre production. Tonnages and shares are for 2024, of about 132 million tonnes of fibre of every kind (Textile Exchange, page 11).
| Fibre | Other names on labels | The polymer | Typical uses | Made in 2024 |
|---|---|---|---|---|
| Polyester | PES; trade names Dacron, Terylene | Almost always PET, polyethylene terephthalate | Shirts, dresses, suits and sportswear, alone or blended with cotton or viscose; fleece; filling; bottles share the polymer | 77.7 Mt, 59% of all fibre |
| Nylon | Polyamide, PA; nylon 6 and nylon 6,6 | A polyamide, held together by amide links | Hosiery, swimwear, outdoor wear, carpets, ropes, airbags and tyre cord | 7.0 Mt, about 5% |
| Polypropylene | Olefin in the US; PP | A polyolefin, made from propylene | Carpets, nonwovens, ropes, technical textiles | 3.2 Mt, about 2.4% |
| Acrylic | PAN; modacrylic is a related fibre | At least 85% acrylonitrile | Knitwear, blankets, fake fur, awnings | 1.6 Mt, about 1.2% |
| Elastane | Spandex in the US; brand Lycra | At least 85% segmented polyurethane | Stretch in jeans, swimwear, hosiery and sportswear, always blended | 1.5 Mt, about 1.1% |
Smaller, specialised synthetics include the aramids (Kevlar for strength, Nomex for heat and flame), ultra-high-molecular-weight polyethylene (Dyneema and Spectra), modacrylic, chlorofibres such as PVC (see vinyl fibres), PTFE and PBI. Polylactide (PLA) is a synthetic polymer made from plant sugars rather than oil: the polymer is synthesised, so the fibre counts as synthetic even though its raw material is renewable.
Name two man-made fibres: polyester and nylon are the two most made, and both are synthetic. If the question wants one synthetic and one regenerated fibre, polyester and viscose rayon.

Is it synthetic? Nylon, rayon, spandex, bamboo, acetate
- Nylon: yes, synthetic. US law defines it as a manufactured fibre of “a long-chain synthetic polyamide” (16 CFR 303.7(i)). The American Chemical Society calls it “the first totally synthetic fiber to be fashioned into consumer products” (ACS).
- Polyester: yes, synthetic, and by far the most made.
- Rayon and viscose: man-made but not synthetic. US law defines rayon as “a manufactured fiber composed of regenerated cellulose” (16 CFR 303.7(d)). The rayon page explains why it is often loosely called semi-synthetic.
- Bamboo fabric: usually viscose rayon made from bamboo pulp, so man-made but not synthetic. The FTC’s guidance is that it must be labelled rayon, or rayon made from bamboo, unless it is made of actual bamboo fibre (FTC, How to Avoid Bamboozling Your Customers).
- Acetate and triacetate: man-made from cellulose, so regenerated rather than synthetic, although the cellulose is chemically changed.
- Spandex, elastane, Lycra: one synthetic fibre under three names, at least 85% segmented polyurethane (16 CFR 303.7(k); EU Annex I). Lycra is a brand.
- Acrylic: synthetic, at least 85% acrylonitrile by weight (16 CFR 303.7(a)); sometimes sold as an “artificial wool”.
- Microfibre: not a fibre type but a fineness, usually under 1 decitex per filament, and almost always polyester or nylon. See microfibre production.
How synthetic fibres are made
Every synthetic fibre is made in two stages: first the polymer, then the fibre. The polymer is usually made at the same plant that spins it (US EPA, AP-42 6.9). Polyester, for example, is made from purified terephthalic acid and ethylene glycol; nylon 6 from caprolactam; nylon 6,6 from hexamethylenediamine and adipic acid; acrylic from acrylonitrile; polypropylene from propylene. The polyester and nylon pages give each route in detail.
The fibre is formed by “forcing a viscous fluid or solution of the polymer through the small orifices of a spinnerette” and solidifying the filaments at once. Which method is used depends on “the polymer’s melting point, melt stability, and solubility” (US EPA, AP-42 6.9):
| Spinning method | How the filament sets | Fibres made this way |
|---|---|---|
| Melt spinning | The polymer is melted, extruded “into a relatively cooler air stream that solidifies the filaments”. No solvent is used | Polyester, nylon 6, nylon 6,6, polyolefins |
| Dry spinning | The polymer is dissolved in an organic solvent and extruded into heated gas, where the solvent evaporates; 94 to 98% of spinning solvent is recovered | Acrylic, modacrylic, vinyon, spandex (and the cellulose acetates) |
| Wet spinning | The polymer solution is extruded into a bath containing a coagulant, where the fibre precipitates | Acrylic, modacrylic |
| Reaction spinning | Prepolymers and monomers react and cross-link after the filament is formed | Spandex |
The freshly spun filaments are weak and stretchy, so they are drawn (stretched) to line up the polymer chains, which gives the fibre its strength. After that comes any of “drawing, lubrication, crimping, heat setting, cutting, and twisting”, and the product leaves the plant as tow, staple fibre or continuous filament yarn; a melt-spun filament yarn “typically is composed of between 15 and 100 filaments” (US EPA, AP-42 6.9). Staple fibre is cut to the length of cotton or wool so that it can be spun on the same machinery and blended with them. The site’s page on the manufacturing of man-made fibres covers the spinning plant in more detail.
Properties of synthetic fibres
Synthetic fibres differ from one another, but they share four traits that set them apart from cotton, wool and viscose:
- They take up little water. Polyester’s commercial moisture regain is 0.4% and polypropylene’s is nil, against 7.0% for raw cotton and 11.0% for rayon. They dry quickly and keep their strength wet, but they feel clammy in heat, build up static and are harder to dye.
- Most are thermoplastic. They soften and then melt: polypropylene at 160 to 175 °C, nylon 6 at about 215 °C, polyester at 250 to 260 °C. Heat sets permanent pleats and creases, and textured yarns, but a hot iron can glaze or hole the fabric. Acrylic is the exception among the big five: it does not melt cleanly but decomposes.
- They are strong and hard-wearing, and the producer can set the strength, fineness, cross-section and lustre by grade. The same strength makes polyester pills stay on the fabric: “owing to the high strength of polyester fibers, these balls or pills cannot drop off, but remain on the surface” (Trevira, US 7,189,794 B2).
- Insects and mould leave them alone, and they do not rot. That is an advantage in use and a problem at the end of life, because they persist (environment).
| Fibre | Density, g/cm³ | Commercial moisture regain, % | EU agreed allowance, % | Effect of heat, °C | LOI, % |
|---|---|---|---|---|---|
| Polyester (PET) | 1.36–1.41 | 0.4 | 1.5 | Melts at 250–260 | 20–21 |
| Nylon 6,6 | 1.14 | 4.5 | 6.25 staple; 5.75 filament | Melts at 255–265 | 20–21.5 |
| Nylon 6 | — | 4.5 | 6.25 staple; 5.75 filament | Melts at about 215 | 20–21.5 |
| Polypropylene | 0.90–0.92 | 0 (as olefin) | 2 | Melts at 160–175 | 18.6 |
| Acrylic | — | 1.5 | 2 | Glass transition about 100; decomposes about 290 | 18.2 |
| Elastane (spandex) | — | 1.3 | 1.5 | — | — |
| Viscose (rayon), regenerated | 1.52–1.54 | 11.0 (as rayon) | 13 | Does not melt; pyrolysis at about 350 | 18.9 |
| Cotton, natural | 1.50–1.56 | 7.0 raw; 8.5 mercerised | 8.5 | Does not melt; decomposes rapidly above 246 | 18–18.5 |
| Wool, natural | 1.30–1.31 | 13.6 | 17 carded; 18.25 combed | Does not melt; chars at about 300 | 23.6–25 |
Two figures in the table explain a lot. Polypropylene’s density is below 1.0, so it floats on water, which suits ropes and nets. And the limiting oxygen index (LOI), the share of oxygen a fibre needs in the air to keep burning, is around 18 to 21 for the common synthetics, so they burn in normal air (21% oxygen); modacrylic and the aramids are the flame-resistant synthetics. The LOI predictor estimates what a flame-retardant finish adds.
Worked example: why a blend is not billed at one fibre’s regain. Water content changes what a consignment weighs, so yarn is sold at an agreed regain. A 50/50 viscose/polyester yarn mixes a fibre allowed 13% with one allowed 1.5%. Take 1,000 kg as received, measured at 6.0% regain. In the blended yarn invoice weight calculator the oven-dry mass is 943.40 kg and holds 56.60 kg of water; the blend’s agreed regain is 7.25%, so the commercial invoice weight is 1,011.79 kg, 11.79 kg more than was weighed. Billing the same yarn at viscose’s 13% would charge for water that is not there; billing it at polyester’s 1.5% would give away yarn.
Advantages and disadvantages of synthetic fibres
| Advantages | Disadvantages |
|---|---|
| Strong, hard-wearing and light for their strength | Absorb little sweat, so feel clammy in heat |
| Dry quickly; keep their strength wet | Build up static |
| Hold heat-set pleats and resist creasing and shrinking | Melt under heat; a hot iron or a spark can hole them |
| Resist moths, mildew and rot | Do not biodegrade; shed microplastic fibres in the wash |
| Made to order: fineness, cross-section, lustre, stretch, flame resistance | Made mostly from oil and gas |
| Made in huge volume, so cheap | Pills stay on the fabric (polyester); oily stains hold |
Much of what blending does in clothing is to trade these columns against those of cotton or viscose: polyester adds strength and crease resistance to a shirting, while the cotton adds comfort and absorbency.
Synthetic vs natural fibres
| Synthetic (polyester, nylon, acrylic, polypropylene) | Natural (cotton, wool, silk, linen) | |
|---|---|---|
| Raw material | Polymers made from oil and gas; PLA from plant sugar | Grown on plants or animals |
| Fibre length | Made as continuous filament; cut to staple when needed | Staple, except silk, which is a filament |
| Water | Regain 0 to 4.5% | Regain 7 to 13.6% (cotton, wool) |
| Heat | Most melt | Char or decompose; do not melt |
| Burn test | Melt and shrink from the flame; leave a hard bead | Burn or char without melting; no hard bead |
| End of life | Persist; can be recycled mechanically or chemically | Biodegrade |
| Share of world fibre, 2024 | 69% (all synthetics) | About 24% plant fibres; about 1% animal fibres |
How to tell if a fabric is synthetic
Read the label first. In the EU and the US the label must name every fibre by its generic name and give its percentage, so “polyester”, “polyamide”, “acrylic”, “elastane” or “olefin” on the label answers the question.
Burn test. Hold a snipped thread in tweezers over a non-flammable dish, away from anything that can catch. Synthetics melt and draw back from the flame and leave a hard bead; nylon’s residue is “initially a hard, cream-colored bead that becomes darker” (FabricLink). Acrylic “burns readily with smoky flame and acid smell. The ash is hard” (CAMEO, as quoted on the acrylic page). Cotton and viscose burn like paper and leave soft ash, which is the quickest way to tell rayon from a synthetic. The site’s fibre identification tests list the others.
Microscope and solvents. Under the microscope most synthetics are smooth, even rods with a round, trilobal or other engineered section, unlike the twisted ribbon of cotton or the scales of wool: see the microscopic appearance of fibres. Laboratories measure the proportions in a blend by dissolving one fibre and weighing what is left, by the parts of ISO 1833: formic acid dissolves polyamide (ISO 1833-7), and dimethylformamide dissolves acrylic (EU Annex VIII, method 8).
Worked example: is the label within tolerance? Both the EU and the US allow 3 percentage points of the total fibre weight between the label and the test (16 CFR 303.43; Regulation 1007/2011, Article 20(3)). A shirt labelled 65% polyester, 35% cotton tests at 61.5% polyester and 38.5% cotton. The fibre content tolerance calculator sets polyester’s band at 62.00 to 68.00%: the shirt is 3.50 points off on both fibres, 0.50 points outside the tolerance, so the label is wrong.
What synthetic fibres are used for
- Clothing: polyester in shirts, dresses, suits, linings, fleece and sportswear, often blended with cotton or viscose; nylon in hosiery, swimwear, lingerie and outdoor shells; elastane for stretch, a few per cent in a blend; acrylic in sweaters, socks and knitted jersey.
- Home textiles: carpets (nylon and polypropylene), upholstery, curtains, blankets (acrylic), and polyester fibre filling for pillows and duvets.
- Ropes and nets: nylon for strength and stretch, polyester for low stretch, polypropylene because it floats, and ultra-high-molecular-weight polyethylene for the highest strength (the fibre-list table puts Spectra at 282 to 327 cN/tex).
- Technical textiles: nylon 6,6 for airbags and tyre cord, because it holds its shape at higher temperatures (Asahi Kasei, 2018); polypropylene and polyester nonwovens in hygiene products, filters and geotextiles; aramids in protective clothing; polyester belts and hoses.
How much synthetic fibre is made
Synthetic fibres “have dominated the fiber market since the mid-1990s”. In 2024 the world made a record 132 million tonnes of fibre, up from 125 million in 2023 and 58 million in 2000, and synthetics were about 91.0 million tonnes of it (Textile Exchange, Materials Market Report 2025, pages 10 and 11). The report puts most of the growth down to new fossil-based synthetics.
| Fibre group, 2024 | Million tonnes | Share of all fibre |
|---|---|---|
| Synthetic fibres | about 91.0 | about 69% |
| of which polyester | 77.7 | 59% |
| of which polyamide (nylon) | 7.0 | 5% |
| of which polypropylene | 3.2 | 2.4% |
| of which acrylic | 1.6 | 1.2% |
| of which elastane | 1.5 | 1.1% |
| Plant fibres (cotton 24.5) | 31.3 | 24% (cotton 19%) |
| Man-made cellulosic fibres (viscose 6.7) | 8.4 | 6% |
| Animal fibres (mostly wool) | about 1.3 | about 1% |
| All fibre | about 132 | 100% |
If business continues as usual, the same report expects 169 million tonnes of fibre in 2030. For polyester’s raw-material prices, see the site’s polyester staple fibre and PTA price series; there is no series yet for nylon, acrylic or polypropylene.
Synthetic fibres and the environment
Raw material. Textile Exchange counts about 62% of all the fibre made in 2024 as fossil-based synthetics, that is synthetics other than recycled and bio-based ones (Materials Market Report 2025, page 12).
Recycling. About 7.6% of all fibre was recycled in 2024, mostly polyester made from plastic bottles, and less than 1% came from recycled textiles. Recycled content differs widely by fibre: about 12.0% of polyester (98% of it from bottles), about 3% of elastane, 2% of nylon, 0.8% of acrylic and 0.4% of polypropylene (same report, page 13). See recycled polyester.
Microfibres. Synthetic fabrics shed fibre fragments in the wash that are small enough to pass through treatment plants. A University of Plymouth study estimated that a 6 kg wash load could release 728,789 fibres from acrylic fabric, 496,030 from polyester and 137,951 from polyester-cotton (Napper and Thompson, Marine Pollution Bulletin 112, 2016). By mass, a study of 37 fabrics measured 161 ± 173 mg of fibre per kg of polyester fabric per wash, against 27 ± 14 mg/kg for nylon (Vassilenko et al., PLoS ONE, 2021).
Worked example: one garment’s lifetime shedding. Take a 250 g polyester top shedding 161 mg/kg in its first wash, declining 3% a wash, washed 50 times with no filter. The microplastic shedding calculator gives 40.25 mg in the first wash and 1,049.10 mg over the garment’s life, 0.42% of its mass. At nylon’s 27 mg/kg the same garment sheds 175.94 mg. The 3% decline is an assumption for the example, not a measured figure. The site’s article on microplastics from synthetic fabrics covers filters and fabric design.
How to wash and iron synthetics
Follow the care label: the number in the wash tub is the maximum temperature, and the dots in the iron set the maximum sole-plate temperature. GINETEX, the international care-labelling association, assigns one dot, 120 °C, to “polyacryl, polyamide (nylon), acetate”, and two dots, 160 °C, to the “wool/silk/polyester/viscose” setting (GINETEX care symbols, following ISO 3758). Because synthetics are thermoplastic, the risks are heat: a hot iron, a hot tumble dryer or a spark can glaze, shrink or hole them, and a crease set in by heat is hard to remove. They dry fast on a line. Polypropylene has the lowest melting point of the five, so it needs the coolest setting, if it is ironed at all.
A short history
| Year | What happened | Source |
|---|---|---|
| 1935 | Wallace Carothers’s group at DuPont makes “fiber 66”, nylon 6,6, on 28 February | ACS landmark |
| 1938 | Paul Schlack polymerises caprolactam in Germany: nylon 6, sold as Perlon. DuPont announces nylon on 27 October | Nylon page |
| 1939–1940 | Nylon production starts at Seaford, Delaware, on 15 December 1939; nylon stockings go on national sale on 15 May 1940 | ACS landmark |
| 1941 | John Rex Whinfield and James Tennant Dickson discover polyester (PET) at the Calico Printers’ Association | Science Museum Group |
| 1950 | Orlon becomes the first commercially manufactured acrylic fibre | CAMEO, Orlon |
| 1951–1953 | Dacron polyester suits go on sale in the US on 8 May 1951; ICI’s Terylene plant at Wilton opens in 1952; DuPont’s Kinston plant in 1953 | Hagley; Wilton International |
| 1958 | DuPont’s “Fiber K”, later Lycra spandex, from the chemist Joseph Shivers | National Inventors Hall of Fame; The LYCRA Company |
| Mid-1990s | Synthetic fibres become the largest fibre group | Textile Exchange |
| 2024 | Synthetics reach about 91 million tonnes, 69% of all fibre | Textile Exchange |
More dates, including the regenerated fibres that came first, are on the timeline of man-made fibres and in the history of natural and man-made fibres.
Related on this site
- The fibres one by one: polyester, nylon, acrylic, polyolefin (polypropylene), spandex (elastane), aramid, vinyl fibres, carbon fibre
- The man-made fibres that are not synthetic: rayon and viscose, regenerated cellulose fibres, regenerated protein fibres, man-made mineral fibres
- Types of textile fibres: the classification and a property table of 34 fibres
- Manufacturing of man-made fibres and polymer fibres
- Calculators: blend invoice weight, moisture regain, fibre content tolerance, microplastic shedding, heat-setting time and temperature, pilling index, LOI predictor, count converter
Sources and corrections
- Production and recycling: Textile Exchange, Materials Market Report 2025, pages 10 to 13.
- Definitions: 15 U.S.C. 70; 16 CFR 303.7 and 303.43; Regulation (EU) No 1007/2011, Annexes I, VIII and IX and Article 20; ISO 2076:2021; FTC, How to Avoid Bamboozling Your Customers.
- Manufacture: US EPA, AP-42, Compilation of Air Pollutant Emission Factors, section 6.9, Synthetic Fibers (9/90, reformatted 1/95).
- Properties: the sources keyed in the site’s fibre property table; Trevira, US 7,189,794 B2; Asahi Kasei, 2018.
- Identification and care: FabricLink burn test; CAMEO, Museum of Fine Arts Boston (archived copy); GINETEX, care symbols.
- Microfibres: I. E. Napper and R. C. Thompson, Marine Pollution Bulletin 112 (2016); E. Vassilenko et al., PLoS ONE 2021 (PMC8270180).
- History: American Chemical Society, Foundations of Polymer Science: Wallace Carothers and the Development of Nylon (archived copy); Science Museum Group; Hagley Museum and Library; Wilton International; National Inventors Hall of Fame; The LYCRA Company (the producer’s own history).
Change log. 18 November 2026: rewritten in full, with this site’s separate page on synthetic fibres folded in. Corrected from the previous versions: rayon was listed among the synthetic fibres (it is regenerated cellulose); glass and rubber were listed among the regenerated fibres; “Polyester” was given as a trade name for nylon; nylon was said to have been invented in 1931 (the fibre was first made in 1935) and by DuPont “in 1938” (the year it was announced); and synthetic fibres were described as thermosetting (they are thermoplastic). Removed because no source was found: a claim that microfibres are “60 times thinner than a human hair”, and a museum-storage section whose source could not be read. Much of the old text closely followed a published museum conservation leaflet; it has been replaced.
Found an error? Please tell us through the contact page, naming the section and the source that disagrees.









WOW just what I was searching for. Came here by searching for meta_keyword|
It’s actually a great and helpful piece of info. I’m happy that you shared this useful info with us. Please keep us informed like this. Thank you for sharing.|