Jump to a calculator 671 tools
Knitting Quality Development
Loop Length for a Target Finished Weight, Through Finishing Shrinkage
Set the loop for the finished fabric. The greige weight is a consequence, not a target.
Loop Length to Set
— mm
Solved at the finished stitch density
Greige Expectation & Finishing Gain
- Greige Weight to Expect
- — g/m2
- Weight Gained in Finishing
- — %
- Tightness Factor at This Loop
- —
- Greige Courses
- — /cm
- Greige Wales
- — /cm
- Area Shrinkage
- — %
- Finished Stitch Density
- — /cm2
- Greige Stitch Density
- — /cm2
- Yarn in a Square Metre
- — m
The shrinkage figures are properties of a quality on a finishing route, not of a fabric type, and must be established from measured greige and finished samples rather than assumed - they drift with relaxation time, compactor setting and moisture. Weight gain in finishing is not independent of them: it is the reciprocal of the area factor, so if a measured gain contradicts the measured shrinkages, one measurement is wrong. This is a single jersey relation as written; on rib and interlock the stitch density must count loops on both beds or the calculated loop length will be out by a structure-dependent factor of around two. The finished density should come from a conditioned, fully relaxed laboratory sample - a density taken from fabric still under roll tension will produce a loop length that misses the target weight in the light direction. Residual shrinkage after laundering is a separate specification and is not addressed here.
Using this calculator
About the Loop Length for a Target Finished Weight, Through Finishing Shrinkage
The formula
This is the expression the tool evaluates. Every term is named underneath, with the unit it must be supplied in.
loopLength = targetGsm x 100 / ( finishedCourses x finishedWales x tex )The same relation that gives weight from loop length runs backwards without ambiguity, because weight is linear in loop length. There is exactly one loop length that produces a given weight at a given density and count.
greigeCourses = finishedCourses x ( 1 - lengthShrink / 100 )Shrinking the fabric in length puts the same courses into less distance, so courses per centimetre rise. Working backwards from finished to greige therefore multiplies rather than divides, and getting that direction wrong is the classic error here.
greigeGsm = greigeCourses x greigeWales x loopLength x tex / 100The loop length is unchanged - it was set at knitting and finishing cannot alter it. Everything that changes between greige and finished weight is stitch density.
weightGain = 1 / ( ( 1 - lengthShrink / 100 ) x ( 1 - widthShrink / 100 ) ) - 1No yarn is added in finishing. The same mass occupies less area, so grams per square metre rise by exactly the reciprocal of the area factor - which makes the weight gain a check on the shrinkage figures rather than an independent quantity.
| Symbol | Stands for | Unit |
|---|---|---|
loop length | Yarn consumed by one loop, fixed at knitting | mm |
stitch density | Courses per cm multiplied by wales per cm | /cm2 |
compacting | Mechanical over-feeding that forces length shrinkage into the fabric | — |
K | Tightness factor, sqrt(tex) over loop length | — |
How the result is derived
Step by step, from the values you type to the figure on screen.
- The 6 inputs are read from the form on every keystroke: Target Finished Weight, Finished Courses, Finished Wales, Yarn Count, Length Shrinkage in Finishing and Width Shrinkage in Finishing.
- Each value is checked against the accepted range in the input table below. A value outside its range stops the calculation rather than producing a misleading figure — the results blank out and a message appears.
- The validated values are substituted into the expression above, which resolves Loop Length to Set together with every supporting figure in one pass — no value is carried over from a previous entry.
- The supporting outputs — Greige Weight to Expect, Weight Gained in Finishing, Tightness Factor at This Loop, Greige Courses, Greige Wales, Area Shrinkage, Finished Stitch Density, Greige Stitch Density and Yarn in a Square Metre — come from the same pass, so they always describe the same case as the headline figure.
- Results are rounded for display only. The full-precision value is used throughout the chain, so reading a rounded intermediate figure back into the tool by hand can shift the last digit.
What each input means
Where to read each value on the floor, the unit it must be in, and the range the tool accepts.
| Input | Unit | Accepted range | Default | What it means |
|---|---|---|---|---|
| Target Finished Weight | g/m2 | 20 to 900 g/m2 | 175 | |
| Finished Courses | /cm | 2 to 80 /cm | 20 | |
| Finished Wales | /cm | 2 to 80 /cm | 15 | |
| Yarn Count | tex | 2 to 200 tex | 20 | |
| Length Shrinkage in Finishing | % | 0 to 45 % | 14 | Relaxation plus compacting |
| Width Shrinkage in Finishing | % | 0 to 45 % | 6 |
What the tool returns
The headline figure and every supporting value it is built from.
| Output | Unit | What it tells you |
|---|---|---|
| Loop Length to Set (headline result) | mm | Solved at the finished stitch density |
| Greige Weight to Expect | g/m2 | |
| Weight Gained in Finishing | % | |
| Tightness Factor at This Loop | — | |
| Greige Courses | /cm | |
| Greige Wales | /cm | |
| Area Shrinkage | % | |
| Finished Stitch Density | /cm2 | |
| Greige Stitch Density | /cm2 | |
| Yarn in a Square Metre | m |
Worked example
Given
- 0
- Target 175 g/m2 finished
- 1
- Finished at 20 courses and 15 wales per cm
- 2
- 20 tex yarn
- 3
- 14% length and 6% width shrinkage in finishing
Substituting
loop = 175 x 100 / ( 20 x 15 x 20 ) = 2.9167 mmgreigeCourses = 20 x 0.86 = 17.2, greigeWales = 15 x 0.94 = 14.1greigeGsm = 17.2 x 14.1 x 2.9167 x 20 / 100 = 141.47gain = ( 175 - 141.47 ) / 141.47 = 23.7011%check: 1 / ( 0.86 x 0.94 ) - 1 = 23.70%Answer
- 0
- Loop length 2.9167 mm, tightness factor 1.5333
- 1
- Greige fabric at 17.2 courses and 14.1 wales per cm
- 2
- Greige weight 141.47 g/m2
- 3
- 23.7011% weight gained through finishing
- 4
- Area shrinks 19.16%; a square metre holds 87,500 m of yarn
The last line is the check worth keeping. Weight gain in finishing must equal the reciprocal of the area factor, because finishing adds no yarn - so if a mill measures a 24% area shrinkage and a 35% weight gain, one of the two measurements is wrong and it is usually the weight, taken from a sample cut before the fabric had fully relaxed. The two numbers are the same number.
How to use it
- Work through the input groups in order — Finished Specification and Finishing Movement. The defaults are a realistic case, so you can change one value at a time and watch what moves.
- There is no calculate button. Every figure recalculates as you type or drag, which is what makes this usable for a what-if sweep rather than a single answer.
- Read Loop Length to Set in the dark results panel — that is the headline figure, expressed in mm.
- Check the supporting rows underneath (Greige Weight to Expect, Weight Gained in Finishing, Tightness Factor at This Loop, Greige Courses, Greige Wales, Area Shrinkage, Finished Stitch Density, Greige Stitch Density and Yarn in a Square Metre) before acting on the headline — they are where an implausible input usually shows itself first.
- Reset to defaults returns every field to the reference case, which is the quickest way to check whether a surprising result came from the tool or from an input you had changed earlier.
Where this is used
- Process planning — establishing Loop Length to Set before a trial is booked, so machine time and material in Knitting, Hosiery & Stretch-Fabric Control are committed against a calculated figure rather than an estimate.
- Costing and quotation — Loop Length to Set is an input to the cost sheet, and quoting from a worked number rather than a remembered one is what keeps a margin intact.
- Troubleshooting — when the floor result drifts from plan, entering the measured values (starting with Target Finished Weight) shows how much of the gap in Loop Length to Set each variable explains.
- Teaching and study — the accepted ranges bracket normal Knitting, Hosiery & Stretch-Fabric Control practice, so moving one variable at a time shows the shape of the relationship rather than a single answer.
Reading the result
Typical bands and what each one is telling you.
| Value | What it indicates |
|---|---|
| K 1.40 - 1.55 | The workable band for cotton single jersey. Outside it, revisit the density or the count. |
| Length shrinkage 10 - 18% | Normal for a relaxed and compacted cotton single jersey. |
| Width shrinkage 4 - 10% | Typical; higher usually means the greige width was forced on the stenter. |
| Weight gain 18 - 28% | Consistent with those shrinkages. A gain outside it contradicts them. |
Assumptions and limits
- The shrinkage figures are properties of a quality on a finishing route, not of a fabric type, and must be established from measured greige and finished samples rather than assumed - they drift with relaxation time, compactor setting and moisture. Weight gain in finishing is not independent of them: it is the reciprocal of the area factor, so if a measured gain contradicts the measured shrinkages, one measurement is wrong. This is a single jersey relation as written; on rib and interlock the stitch density must count loops on both beds or the calculated loop length will be out by a structure-dependent factor of around two. The finished density should come from a conditioned, fully relaxed laboratory sample - a density taken from fabric still under roll tension will produce a loop length that misses the target weight in the light direction. Residual shrinkage after laundering is a separate specification and is not addressed here.
- Every input is bounded to the range normal practice occupies (Target Finished Weight 20 to 900 g/m2, Finished Courses 2 to 80 /cm and Finished Wales 2 to 80 /cm, and so on for the rest). Those bounds are guard rails against typing errors, not a claim that the formula fails one unit outside them.
- The calculation is deterministic: the same inputs always give the same result. It carries no allowance for machine condition, operator skill, ambient conditions or lot-to-lot material variation unless an input above explicitly represents one.
- Nothing is sent anywhere. The maths runs in your browser, so the numbers you type never leave the page.
Standards and further reading
- ISO 3801 - determination of mass per unit length and mass per unit area.
- ISO 5077 - determination of dimensional change in washing and drying.
- ISO 6330 - domestic washing and drying procedures for textile testing.
- AATCC 135 - dimensional changes of fabrics after home laundering.
Questions people ask
Why not just set the loop from the greige weight?
Because the greige weight is not a specification, it is an outcome - and it is an unstable one. Greige stitch density depends on how long the fabric has been off the machine, whether it has been rolled or plaited, and how much tension it saw on the way, so two samples of the same fabric can measure ten per cent apart in weight while having identical loop length. The customer buys the finished fabric, the finished density is what a conditioned laboratory sample measures, and the loop length is the one quantity that survives the whole route unchanged. Solving at the finished end and reporting the greige figure as an expectation, rather than a target, is the direction that stays true.
What if the greige fabric does not weigh what this predicts?
Check the loop length first, by unravelling, before adjusting anything. If the loop length is right and the greige weight is not, the greige stitch density is not what the shrinkage figures assume, which means either the shrinkage assumption is stale or the greige sample was measured under tension or before relaxing. If the loop length is wrong, the weight discrepancy is explained and the cam or the feeder is the place to look. Adjusting the cam to make the greige weight match a target computed from assumed shrinkage is the wrong response and a common one: it produces a fabric that weighs correctly in greige and misses the finished specification, which is the number that gets paid for.
How stable are the shrinkage figures?
Stable enough for one quality on one finishing route, and not transferable beyond that. Length and width shrinkage depend on the fabric structure, the yarn, the relaxation the fabric is allowed before compacting, the compactor settings and the moisture at which it is set - all of which are properties of a recipe rather than of a fabric type. They should be established from measured greige and finished samples of the quality in question and re-established after any finishing change, and they will still drift with season and machine condition. Treating a shrinkage pair as a fixed property of a quality is why the first bulk lot after a development often misses weight.
Does this work for rib and interlock?
The weight relation holds for any weft-knitted structure provided the density is counted the same way, but there is a trap: on double jersey structures a course of fabric involves loops on both beds, so stitch density counted as visible courses times visible wales on one face undercounts the loops in the fabric by a factor of two for interlock and by a structure-dependent factor for rib. Either count all loops and use this expression unchanged, or use the visible density and expect the calculated loop length to be the sum for both beds. Being explicit about which convention is in use matters more than which one is chosen, because the factor of two is exactly the size of error that gets rationalised as a shrinkage difference.