You cannot prove at home that a shawl is genuine pashmina. The tests sellers suggest, such as burning a thread, pulling the shawl through a ring or rubbing it for static, can expose a synthetic fake, but none of them can tell pashmina from fine sheep’s wool, and none says where or how the shawl was made. Two things can settle it: a laboratory fibre test, or a certification label you can check against a public register. India has registered four pashmina Geographical Indications (GIs), and the oldest, Kashmir Pashmina, has its own tested and numbered label.
This page sets out what each check proves, from the GI Registry’s records, the labelling rules of the US and the EU, and the published test standards. For the fibre itself, its sources and how a shawl is made, see Pashmina Wool Fibers; for the other goat and camel hair fibres, see Hair Fibers: Alpaca, Llama, Cashmere, Mohair and Camel.
What “pashmina” means on a label
In the application that registered the Kashmir Pashmina GI, pashm is the fine under-fleece of the Himalayan goat Capra hircus, and “pashmina” is pashm in its woven form. The same document gives the fibres as 12 to 16 microns thick and never more than 18 (Statement of Case of 9 December 2005, on the GI Registry record for application 46). Outside India, the word is not a fibre name:
- United States. The Federal Trade Commission’s business guide on cashmere (July 2014) calls pashmina an Indian word for cashmere, says it is not a labelling term recognised by the Wool Products Labeling Act, and says a label cannot read “100% Pashmina”. The fibre content must be stated, for example “70% Cashmere, 30% Silk”. Under the Act the hair of the cashmere goat counts as wool (15 U.S.C. 68(b)), and the word “cashmere” may be used only for the fine dehaired undercoat of the cashmere goat with an average diameter of no more than 19 microns, no more than 3 % by weight of fibres averaging over 30 microns, and a coefficient of variation of no more than 24 % (16 CFR 300.19; see the US wool labelling rules).
- European Union. Only the names in Annex I of Regulation (EU) No 1007/2011 may describe fibre content. “Cashmere” is the hair of the Kashmir goat; “pashmina” is not on the list (Article 5 and Annex I). The same entry names cashgora separately, so cashgora is not cashmere on an EU label. “100 %” is allowed only for a product made of one fibre, with up to 2 % of technically unavoidable extraneous fibres, or 5 % after carding (Article 7; see the EU Textile Labelling Regulation).
- India. The Indian Standard for identifying and labelling pashmina is IS 17269, described below.
So a label that says “100% pashmina” and nothing else does not meet the US or EU rules, and the EU rule sets no diameter at all. A shawl sold there as cashmere still has to be cashmere, but the law does not say how fine.
India’s four registered pashmina GIs
A GI ties a name to goods from one place, made in a set way. The GI Registry’s public records, read on 10 October 2026, show four registered pashmina GIs. The list of registered GIs published by Intellectual Property India gives the same four.
| GI (application) | Registered proprietor | Goods class | Filed and certified | Valid until | Authorised users listed |
|---|---|---|---|---|---|
| Kashmir Pashmina (46) | TAHAFUZ, a society registered under the J&K Societies Act, Srinagar | 23, 24, 25 | Filed 9 Dec 2005; certificate No. 97 of 12 Sep 2008 | 8 Dec 2025 on the record; renewal fee receipted 30 Jun 2025 | 1,662 (1,176 marked Registered) |
| Pashmina Wool of Ladakh (726) | Ladakh Autonomous Hill Development Council, Leh | 22 | Filed 8 Dec 2020; certificate No. 466 of 31 Mar 2023 | 7 Dec 2030 | None |
| Basohli Pashmina Woolen Products (775) | Sahib Pashmina Handloom Weaving Industrial Cooperative, Basohli, Kathua | 24, 25 | Filed 9 Aug 2021; certificate No. 507 of 3 Oct 2023 | 8 Aug 2031 | None |
| Ladakh Pashmina Textile (1386) | Directorate of Industries and Commerce, UT of Ladakh, with Looms of Ladakh Women Cooperative | 24 | Filed 26 Nov 2024; certificate dated 28 Mar 2026, number not shown | Not shown | None |
Under the Geographical Indications of Goods (Registration and Protection) Act, 1999, the authorised users of a registered GI have the exclusive right to use it on the goods it covers (section 21(1)(b)). Selling goods that carry a false GI is an offence punishable with six months to three years in prison and a fine of 50,000 to 2 lakh rupees, either of which a court may lower for special reasons, unless the seller proves one of the section’s defences, such as having taken all reasonable precautions (section 40). For a buyer, that makes the GI the one pashmina claim with a public register behind it: ask which GI the seller means, then look for the seller among the authorised users on that GI’s record. On 10 October 2026 only Kashmir Pashmina had any authorised users listed.
What the Kashmir Pashmina label looks like
The proprietor, TAHAFUZ, filed a Quality Manual on the GI Registry record for application 46 on 25 March 2019. It limits the GI to goods made of 100 % pashm, hand spun and hand woven by artisans of Jammu and Kashmir, and it describes the label:
- a round label with a serrated edge, 2.5 centimetres across, called a Secure Fusion Authentication Label;
- visible text: “Kashmir Pashmina”, the registered GI logo, “Certified Genuine” and a unique number, which records the authorised user it was issued to;
- hidden text, “Registered GI” and “100% Handmade”, readable under ultraviolet light, and invisible marker particles readable with an infrared device;
- on shawls, stoles, mufflers and scarves, placed 4.5 inches from the end, lengthwise;
- only on finished goods, only after testing, and never on a made-up item that combines pashmina with any other material. A pashmina and silk blend cannot carry it.
The manual’s tests are carried out by a laboratory the proprietor appoints; it names the Pashmina Testing and Quality Certification Centre on the CDI campus at Nowshera, Srinagar.
| Parameter | Instrument | What it checks |
|---|---|---|
| Origin of fibre | Differential scanning calorimeter | The fibre’s thermal properties |
| Fineness | Projection microscope | Fibre diameter |
| Spinning | Twist tester | Twist direction: S for hand-spun yarn, Z for machine spinning |
| Weaving | Pick glass | How much the ends and picks vary across the piece |
The manual gives no pass mark for the thermal, twist or weaving tests. It tests 10 % of the items in a lot, rounded up, and refuses the whole lot if one sample fails. A label therefore shows that the piece came from a lot that passed sampling, not that the piece itself was tested.
India’s standard: IS 17269
The Bureau of Indian Standards’ catalogue entry lists IS 17269:2021, Identification, Labelling and Marking of Pashmina Products, the first revision of the 2019 edition, with one amendment, from the Wool, Wool Products and Textile Floor Coverings Sectional Committee (TXD 04). It refers to IS 744:2000, the Indian method for wool fibre diameter, medullated fibres and kemp. When BIS announced the 2019 edition on 9 August 2019, it said the standard covers raw fibre, yarn, sliver, fabric and finished products of 100 % pashmina and of pashmina blended with sheep or merino wool and other speciality fibres, with silk, with cellulosic fibres or with synthetics.
The standard’s text sits behind a BIS login, so this page does not give its limits. The catalogue entry also showed no licences issued against IS 17269:2021 on 10 October 2026. If a seller claims BIS certification for a pashmina product, ask for the licence number.
What a laboratory test can prove
Two international methods cover the question a buyer is really asking: ISO 17751-1:2023, by light microscopy, and ISO 17751-2:2023, by scanning electron microscopy, both second editions published in July and August 2023. Each identifies cashmere, sheep’s wool and other speciality animal fibres and measures their proportions, in loose fibre, intermediate products or finished products (records: ISO 17751-1, ISO 17751-2). A lab report on one of these methods can show:
- whether the “pashmina” is cashmere at all, or sheep’s wool, or another hair fibre;
- how much of each is present, which is what a fibre content label has to state.
A laboratory can also measure the mean fibre diameter, the figure the US definition of cashmere turns on, by a method such as IS 744, which IS 17269 cites.
Their stated scope is fibre type and proportion. Neither method claims to name the region a fibre came from or to tell hand-spun from machine-spun yarn, which is why the Kashmir Pashmina manual adds a thermal test for origin and a twist test for spinning. A test needs a cutting from the shawl, so ask a seller for an existing report before you buy.
How to tell genuine pashmina at home, and what home tests miss
| Check | What it can show | What it cannot show |
|---|---|---|
| Burn a fringe thread | Whether the fibre is protein, plant or synthetic. Cashmere, wool and silk smell of burnt hair and leave a crushable ash; cotton and viscose burn like paper; polyester, nylon and acrylic melt into hard beads | Cashmere from sheep’s wool, yak or silk: all are protein fibres and burn alike. A blend can show both behaviours in one thread |
| Pull it through a ring | That the fabric is fine and light | The fibre. A fine wool, silk or viscose shawl passes; a thicker genuine shawl may not |
| Rub it for static | Almost nothing | The fibre: static depends on the air’s humidity as much as on the fabric |
| Look for pilling | Nothing either way | Genuineness: fine short fibres pill, and so do cheap blends |
| Read the fibre label | What the seller declares, such as cashmere and its percentage | Whether the declaration is true |
| Look at a fringe yarn’s twist under a magnifier | Whether it is S twist, where the spiral slopes like the middle stroke of the letter S, the direction the GI manual expects of hand-spun yarn | The fibre, or proof of hand spinning: a machine can spin S twist too |
| Check a GI label | The label’s shape, size, wording and number; the seller’s name on the GI record | The hidden marks, which need ultraviolet and infrared readers |
A burn test is the only home test that rules anything out, and it only rules out a synthetic or plant fibre. Everything else on the list is about the fabric, not the fibre.
Reading a lab report against the label
A retailer or importer is more likely to hold a lab report than to burn a thread. Take a stole sold in the EU, labelled “70 % cashmere, 30 % silk”, and a report that finds 67.4 % cashmere and 32.6 % silk. The EU allows a manufacturing tolerance of 3 % between the label and the analysis, in relation to the total weight of fibres (Article 20(3)), which is three percentage points either way, not 3 % of the figure declared. In the fibre content tolerance calculator, enter the declared and found figures, leave the third fibre at zero and set the tolerance to 3:
- the deviations are −2.6 points for cashmere and +2.6 for silk, so the largest is 2.6;
- the band for cashmere is 67 to 73 %, and the margin against the tolerance is 0.4 points, so neither fibre is outside it. Open the calculator with this report.
- Read as 3 % of 70, the band would be 67.9 to 72.1 % and the same report would wrongly fail.
- Had the report said 66.4 % cashmere and 33.6 % silk, the largest deviation would be 3.6, the margin −0.6, and both fibres would be outside the band: open it with 66.4.
Two limits. Do not use the calculator for a “100 %” claim under EU rules: it applies a band of zero to a single-fibre claim, while Article 7 allows the 2 % or 5 % of extraneous fibres described above. And in the US, cashmere goods are wool products, for which the law sets no fixed figure: a deviation from the label is excused only if the seller proves it came from unavoidable variation in manufacture despite due care (15 U.S.C. 68b(a)(2)(A)). The calculator’s default of 3 points comes from the US Textile Act rule, 16 CFR 303.43, not from the wool law.
Shahtoosh is not a grade of pashmina
Shahtoosh is the fine wool of the Tibetan antelope, Pantholops hodgsonii, also called the chiru. CITES has listed the species in Appendix I since 28 June 1979, after Appendix II from 1 July 1975 (CITES listing history). Its Resolution Conf. 11.8 (Rev. CoP17) recommends that every Party treat any product claimed to be shahtoosh, or claimed to contain Tibetan antelope, as a recognisable part or derivative of the species, subject to the Appendix I rules. In India the Tibetan antelope is in Schedule I, Part A of the Wild Life (Protection) Act, 1972, as substituted by the Wild Life (Protection) Amendment Act, 2022, in force from 1 April 2023. A shawl offered as shahtoosh, or as a shahtoosh blend, is offered as the product of a protected wild animal, whatever it contains. It is not a finer pashmina.
How this page is kept
Last verified: 10 October 2026. GI facts come from the GI Registry’s records for applications 46, 726, 775 and 1386 and the documents filed on them, including the Kashmir Pashmina Statement of Case (2005) and Quality Manual (2019); the GI Act from its consolidated text; IS 17269 from BIS’s catalogue and its 2019 announcement, not from the standard’s text, which this page has not read; the ISO methods from ISO’s catalogue; the label rules from the FTC’s guide, 16 CFR 300.19 as published on 1 October 2026, 15 U.S.C. 68 and 68b, and Regulation (EU) No 1007/2011 as consolidated on 15 February 2018; and the shahtoosh listings from Species+, the CITES resolution and the Gazette of India. Each is linked where it is used. Authorised-user and licence counts change, so check the registers themselves. This page describes what the records and rules say; it is not legal advice or a test result for any product. Corrections are welcome through the contact page.