Home » Quality & Testing » Textile Testing Standards: ISO, AATCC and ASTM Methods for Each Test

Textile Testing Standards: ISO, AATCC and ASTM Methods for Each Test

ISO, AATCC and ASTM write most textile test methods. This page pairs them test by test, from colour fastness and shrinkage to tensile strength and pilling.

Laboratory technicians in hair nets, masks and safety glasses pipetting blue liquid into a flask beside racks of test tubes and a microscope

Textile testing standards are published test methods that tell a laboratory exactly how to measure one property of a fibre, yarn, fabric or garment, so that two laboratories testing the same cloth get results that can be compared. Three bodies write most of the methods named on specifications and test reports: ISO, the International Organization for Standardization, through its technical committee ISO/TC 38 Textiles; AATCC, the American Association of Textile Chemists and Colorists, whose methods concentrate on colour fastness, wet testing and chemical analysis; and ASTM International, whose Committee D13 on Textiles covers physical properties. Most common tests have an ISO method and an AATCC or ASTM counterpart: colour fastness to washing is ISO 105-C06 or AATCC TM61, shrinkage is ISO 5077 (with the washing procedures of ISO 6330) or AATCC TM135, fabric tensile strength is ISO 13934-1 or ASTM D5035 by the strip method and ISO 13934-2 or ASTM D5034 by the grab method, pilling is ISO 12945 or ASTM D3512, fibre content is ISO 1833 or AATCC TM20A, and pH is ISO 3071 or AATCC TM81. National bodies adopt many of these under their own prefixes: BS EN ISO in Britain, IS/ISO in India, and GB/T numbers of China’s own. The table below pairs over thirty tests with their methods and links the site’s record of each standard where one is published.

Last verified: 11 October 2026. Standard numbers, current editions and scopes were read that day from the publishers’ own catalogue pages, which are linked in each section and listed at the end. This page names and describes standards; it does not reproduce them. The methods themselves are sold by ISO, AATCC, ASTM and the national standards bodies.

Textile testing standards at a glance: which standard for which test

Read across a row to find the matching method in each family. A dash means that family has no method for the test in this list. Linked numbers open the site’s record of the standard, which keeps its scope, its equivalents and where it is used. Methods in the same row measure the same property but are not interchangeable: specimen size, washing conditions, number of cycles and rating scale can all differ, so a test report has to name the method it followed and a specification has to name the one it requires.

TestISO (TC 38)AATCCASTM (D13)
Conditioning before testingISO 139—D1776/D1776M
Colour fastness to washingISO 105-C06 (domestic and commercial laundering); ISO 105-C10 (soap or soap and soda)TM61 (accelerated laundering)—
Colour fastness to rubbing (crocking)ISO 105-X12TM8 (crockmeter)—
Colour fastness to lightISO 105-B02 (xenon arc)TM16.3 (xenon arc)—
Colour fastness to perspirationISO 105-E04TM15—
Colour fastness to waterISO 105-E01TM107—
Grading colour change and stainingISO 105-A02 and ISO 105-A03 (grey scales)EP1 and EP2 (gray scales)—
Dimensional change (shrinkage) in washingISO 5077, with the procedures of ISO 6330 and the marking of ISO 3759TM135 (fabrics), TM150 (garments)—
Skew and bow—TM179 (skew change after laundering)D3882
Smoothness after launderingISO 7768TM124—
Tensile strength, strip methodISO 13934-1—D5035
Tensile strength, grab methodISO 13934-2—D5034
Tear strengthISO 13937-1 (Elmendorf), -2 (trouser), -3 (wing), -4 (tongue)—D1424 (Elmendorf), D2261 (tongue)
Bursting strengthISO 13938-1 (hydraulic), ISO 13938-2 (pneumatic)—D3786/D3786M (diaphragm), D6797 (ball burst)
Seam strength and seam slippageISO 13935-1 and -2 (seam strength), ISO 13936-1 to -3 (slippage)—D1683/D1683M
PillingISO 12945-1 (pilling box), -2 (modified Martindale), -3 (random tumble), -4 (visual assessment)—D3512/D3512M (random tumble), D3511/D3511M (brush), D4970/D4970M (Martindale)
Abrasion resistanceISO 12947-1 to -4 (Martindale)—D4966 (Martindale), D4157 (oscillatory cylinder), D3884 (rotary platform, a guide)
Fibre identificationISO/TR 11827TM20D276 was withdrawn in 2021
Fibre content of blendsISO 1833-1 and its parts for each fibre mixtureTM20AD629 was withdrawn in 2024
pH of the water extractISO 3071TM81—
FormaldehydeISO 14184-1 (free and hydrolysed), ISO 14184-2 (released)TM112 (released, sealed jar)—
Fabric weight (GSM)ISO 3801 (woven fabrics)—D3776/D3776M
Ends and picks per unit lengthISO 7211-2—D3775
ThicknessISO 5084—D1777
Air permeabilityISO 9237—D737
Water repellency (spray test)ISO 4920TM22—
Water penetration (hydrostatic pressure)ISO 811——
Oil repellencyISO 14419TM118—
Yarn count (linear density)ISO 2060—D1907/D1907M
Yarn breaking forceISO 2062—D2256/D2256M
Burning behaviour of fabricsISO 6940 (ease of ignition), ISO 6941 (flame spread)—D1230 (apparel textiles)
Visual inspection and grading of fabric——D5430
Sampling a lot for inspection (AQL)ISO 2859-1——

Few pairs are declared equivalent by a publisher. AATCC states that TM107 is technically equivalent to ISO 105-E01, TM118 to ISO 14419 and TM124 to ISO 7768, and that TM135 and TM150 are related to ISO 3759. The other rows pair methods that measure the same property in different ways.

Who writes textile testing standards

ISO/TC 38 Textiles

ISO’s textile committee, ISO/TC 38, was created in 1947, and its secretariat is held by SAC, China’s national standards body. Its scope covers fibres, yarns, threads, cords, rope, cloth and other textile materials together with their methods of test, terminology and definitions, the raw materials and chemicals used to process and test them, and specifications for textile products, and it now extends to microplastics from textiles, traceability of animal fibres and ethical and environmental issues in the supply chain. On 11 October 2026 ISO listed 456 published standards for the committee, a count that includes updates, 191 of them under the direct responsibility of TC 38 itself, and 32 more under development.

Most test methods belong to its five subcommittees. SC 1, Tests for coloured textiles and colorants, holds the ISO 105 colour fastness series. SC 2, Cleansing, finishing and water resistance tests, holds ISO 5077, ISO 6330, ISO 3759, ISO 4920 and ISO 811. SC 23, Fibres and yarns, holds ISO 2060 and ISO 2062. SC 24, Conditioning atmospheres and physical tests for textile fabrics, holds ISO 139, ISO 3801, ISO 9237 and the strength, pilling and abrasion series ISO 13934, 13937, 13938, 12945 and 12947. SC 20 covers fabric descriptions. Composition and chemical methods such as ISO 1833, ISO 3071 and ISO 14184 are held by TC 38 directly.

A textile testing laboratory with a vertical strength tester in the foreground, yarn testing instruments and a cone of yarn on a wooden bench, and a technician in a white coat at an instrument at the far end
Yarn and fabric testers in a textile laboratory. Photo published by the North Eastern Handicrafts and Handlooms Development Corporation.

AATCC

The American Association of Textile Chemists and Colorists is a non-profit organisation that has served the textile industry since 1921. In its own description, AATCC methods tend to focus on colour fastness, wet testing and chemical analysis, while ASTM tests evaluate physical properties. The two families are closely tied to ISO’s. AATCC says many ISO colour fastness and water resistance tests were taken directly from AATCC methods: for more than 60 years it was co-secretariat of ISO/TC 38/SC 1 and secretary of SC 2, until it handed both secretariats to other countries in 2010. AATCC and ASTM Committee D13 jointly administer the Technical Advisory Group that represents the United States in ISO/TC 38 (AATCC frequently asked questions).

ASTM Committee D13 on Textiles

ASTM Committee D13 on Textiles was formed in 1914. On 11 October 2026 ASTM gave it 429 members and jurisdiction over 317 standards, published in Volume 07.02 of the Annual Book of ASTM Standards. Its methods are written in subcommittees, among them D13.51 for conditioning, chemical and thermal properties, D13.58 for yarns and fibres, D13.59 and D13.60 for fabric physical test methods, D13.61 for apparel and D13.92 for terminology.

National versions: BS EN ISO, IS/ISO and GB/T

Many countries publish ISO methods as national standards. The British Standards Institution explains that the prefix of a number shows where a standard applies, so the three prefixes in a number such as BS EN ISO 9001 mean it is at once an international, a European and a British Standard (BSI, What is a standard?); textile methods follow the same pattern. India’s Bureau of Indian Standards issues parts of ISO 105 as IS/ISO 105 through its Textiles Department, under the TXD 05 Chemical Methods of Test Sectional Committee (BIS record for IS/ISO 105, part F10). China’s national standards carry numbers of their own: GB/T 3921-2008 carries the English title of ISO 105-C10 apart from the part number, and China’s national standards portal lists it as current and as adopting an international standard. A buyer’s specification decides which of these applies.

How to read a textile standard number

  • ISO. ISO 105-C06:2010 is series 105 (colour fastness), part C06, in the edition published in 2010. In ISO 105 the letter groups the parts, as their titles in ISO’s catalogue show: A for general principles and the grey scales, B for light and weathering, C for washing and laundering, D for dry cleaning, E for water and other wet treatments such as perspiration and sea water, F for the adjacent fabrics used to judge staining, G for atmospheric gases, J for colour measurement, N for bleaching, P for heat, S for vulcanisation, X for other treatments including rubbing, and Z for properties of the dyes themselves. The catalogue listed 94 current parts on 11 October 2026.
  • ISO stage. Each catalogue entry carries a stage code: 60.60 means published, 90.93 confirmed after systematic review, 90.92 to be revised, 90.20 under systematic review and 95.99 withdrawn. An old year is not a sign of a dead standard: ISO 3801:1977 is still the current, confirmed edition.
  • AATCC. AATCC writes its designations as AATCC TM, LP, EP or M, then the number and the year, for example AATCC TM8-2016 or AATCC LP1-2018; TM is a test method, EP an evaluation procedure and LP a laboratory procedure. AATCC notes that since 2020 additional year formats appear, which is why its store lists the accelerated laundering method as AATCC TM61-2013e(2020)e2. You will also see the method cited as AATCC 61, without the TM prefix.
  • ASTM. ASTM textile methods are D numbers. In D5034-21(2025) the 21 is the year of the last revision and the year in brackets is the year of the last reapproval; ASTM’s own identifier for that edition is D5034-21R25.

Latest versions of the most-used standards

As listed by each publisher on 11 October 2026: ISO editions and stages from ISO’s catalogue for TC 38 and its subcommittees, AATCC designations from the AATCC store, ASTM designations from Committee D13’s lists of standards. Check the publisher’s page before relying on an edition, because a confirmed or reapproved standard can be revised at the next review.

StandardCurrent editionStatus on 11 October 2026
ISO 139ISO 139:2005, with Amendment 1:2011Confirmed
ISO 105-A02 / ISO 105-A031993 / 2019Confirmed
ISO 105-B022014To be revised
ISO 105-C062010 (fourth edition)Confirmed
ISO 105-C102006Confirmed
ISO 105-E01 / ISO 105-E042013 / 2013Confirmed
ISO 105-X122016Under systematic review
ISO 37592011Confirmed
ISO 38011977Confirmed
ISO 50772007Confirmed
ISO 63302021Published
ISO 7211-22024Published
ISO 92371995Confirmed
ISO 12945-1 to -42020Review closed
ISO 12947-22016Confirmed
ISO 13934-1 / ISO 13934-22013 / 2014Confirmed
ISO 13935-22026Published
ISO 13937-1 to -42000Confirmed
ISO 13938-1 / ISO 13938-22019Confirmed
ISO 1833-12020To be revised
ISO 30712020Confirmed
ISO 14184-12011Confirmed
ISO 2060 / ISO 20621994 / 2009Confirmed / to be revised
AATCC colour fastnessTM61-2013e(2020)e2; TM8-2016e(2022)e; TM16.3-2020; TM15-2021e; TM107-2022e; EP1-2025; EP2-2025Listed in the AATCC store
AATCC dimensional change and appearanceTM135-2025; TM150-2025; TM179-2025; TM124-2018Listed in the AATCC store
AATCC chemical and repellencyTM20-2021; TM20A-2025; TM81-2022; TM112-2020; TM22-2024Listed in the AATCC store
ASTM fabric strengthD5034-21(2025); D5035-11(2024); D1424-25; D2261-13(2024); D3786/D3786M-18(2023); D6797-24; D1683/D1683M-22Active
ASTM pilling and abrasionD3512/D3512M-22; D3511/D3511M-16(2022); D4970/D4970M-22(2026); D4966-22(2026); D4157-13(2022); D3884-22Active
ASTM construction and conditioningD1776/D1776M-20(2024); D3776/D3776M-20(2025); D3775-17(2023); D737-18(2023); D1777-26; D1907/D1907M-12(2025); D2256/D2256M-21Active
ASTM inspection and flammabilityD5430-26; D1230-25Active

Colour fastness standards: ISO 105 and AATCC

A colour fastness test has two results: the change in colour of the specimen, and the staining of undyed adjacent fabric tested with it. Both are graded against grey scales, ISO 105-A02 for change in colour and ISO 105-A03 for staining, or AATCC EP1 and EP2 in the AATCC system. ISO describes the A02 scale as five steps, each a pair of grey chips or swatches, with an augmented version that adds four half-steps for nine in all. Grade 5 means no change or no staining and grade 1 the most, so a result is reported as a grade such as 4 or 3–4 (AATCC writes the half-steps as decimals, 4.5; AATCC Gray Scales). ISO 105-A05 gives the instrumental route from a colour measurement to a grey scale rating.

Hands holding a grey scale and a masking card against pink fabric specimens inside a grey viewing cabinet
Grading a colour fastness result against a grey scale in a viewing cabinet. Photo published by an instrument maker.
  • Washing. ISO 105-C06 tests resistance to domestic and commercial laundering with a reference detergent. ISO says one single (S) test closely approximates one laundering, and one multiple (M) test may approximate up to five launderings at temperatures not exceeding 70 °C. ISO 105-C10 has five methods, from mild to severe, for washing with soap or soap and soda, and measures the effect of washing alone. AATCC TM61 is an accelerated test: in AATCC’s summary, one 45-minute test roughly approximates five typical hand or home launderings.
  • Rubbing (crocking). ISO 105-X12 and AATCC TM8 both rub a test cloth against the coloured textile, once dry and once wet, and grade the colour transferred to the cloth; AATCC specifies white test cloth. Dry and wet results are graded separately.
  • Light. ISO 105-B02 exposes the specimen to a xenon arc lamp representative of daylight (D65) and judges it against blue wool references; ISO notes that its two permitted sets of references may not give identical results. AATCC TM16.3 offers three xenon-arc options and says the relationship between any lightfastness test and real exposure has to be agreed by the parties.
  • Perspiration and water. ISO 105-E04 tests resistance to human perspiration. AATCC TM15 uses acid perspiration only: AATCC says committee work that correlated with limited field studies led it to drop the alkaline test. For water, AATCC states that TM107 is technically equivalent to ISO 105-E01.

Shrinkage: dimensional change standards

Shrinkage is tested by marking a specimen, washing and drying it by a set procedure, and measuring the marks again. ISO splits the job across three standards. ISO 3759 covers preparing, marking and measuring fabrics and garments. ISO 6330 specifies the domestic washing and drying procedures: 16 for a front-loading reference machine (type A), 12 for a top-loading agitator machine (type B), 7 for a top-loading pulsator machine (type C), and six drying procedures from line dry to tumble dry. ISO 5077 is the method that combines them to give the dimensional change of fabrics, garments or other textile articles. In the AATCC family, TM135 covers fabrics and TM150 garments, each with four washing temperatures, three agitation cycles and four drying procedures; alternative home laundering settings are in AATCC LP1 (machine washing) and LP2 (hand washing). AATCC TM179 measures the change in skew after laundering, and ISO 7768 and AATCC TM124 grade the smoothness of fabric after cleansing.

The result is the change in each marked distance as a percentage of the original. Worked through for a fabric marked at 50 cm in each direction:

MeasurementBefore washingAfter washing and dryingChange
Length marks50.0 cm48.2 cm1.8 ÷ 50.0 × 100 = 3.60% shrinkage
Width marks50.0 cm49.0 cm1.0 ÷ 50.0 × 100 = 2.00% shrinkage
Area10.964 × 0.980 = 0.94475.53% smaller
Fabric weight150 g/m²150 ÷ 0.9447 = 158.78 g/m²5.85% heavier, because the same mass covers less area

Calculator: shrinkage and GSM after washing, set to this example. The calculator shows contraction as a positive shrinkage. The figure means little without the procedure behind it: ISO notes that the machine type, the detergent and the type of tumble dryer can all affect the result, which is why ISO 6330 and TM135 fix those parameters and a report has to name them.

Strength tests: tensile, tear, burst and seams

Tensile. ISO 13934-1 is the strip method for maximum force and elongation at maximum force. It is mainly for woven fabrics, including stretch wovens, is not normally applied to nonwovens, coated fabrics or glass fabrics, and is restricted to constant-rate-of-extension (CRE) machines. ISO 13934-2 is the grab test. ASTM’s pair is D5035 (strip) and D5034 (grab and modified grab). ASTM describes the grab test as suitable for woven, nonwoven and felted fabrics but not recommended for knitted or other high-stretch fabrics (more than 11%), and warns that there is no simple relationship between grab and strip results, because a grab specimen is helped by the yarns beside the ones gripped.

A strength result is the mean of several specimens, and the spread matters as much as the mean. Five grab results of 412, 398, 431, 405 and 420 N average 413.2 N, which clears a 400 N minimum by 13.2 N. But the standard deviation is 12.9 N (a coefficient of variation of 3.1%), the lower end of the 95% confidence interval for the mean is 397.2 N, and one specimen broke below 400 N, so whether the fabric passes depends on how the buyer’s specification is written. Calculator: grab tensile statistics, set to these five results.

Tear. The four parts of ISO 13937 are named by specimen shape: part 1 the ballistic pendulum (Elmendorf) method, part 2 trouser-shaped specimens, part 3 wing-shaped and part 4 tongue-shaped (double tear). ASTM uses D1424 for the falling-pendulum (Elmendorf-type) apparatus and D2261 for the tongue (single rip) procedure on a CRE machine.

Burst. Bursting tests suit knitted fabrics, for which ASTM does not recommend its grab test. ISO 13938-1 uses hydraulic pressure and ISO 13938-2 pneumatic pressure; both apply to knitted, woven, nonwoven and laminated fabrics. ISO notes no significant difference between hydraulic and pneumatic results for pressures up to 800 kPa, the range that covers most apparel, and recommends the hydraulic apparatus for speciality textiles that need higher pressures. ASTM’s methods are D3786/D3786M (diaphragm tester) and D6797 (CRE ball burst).

A pneumatic bursting strength tester with a touch screen, a yellow fabric specimen clamped under a clear test dome, and a green clamp button on each side
A pneumatic bursting strength tester, the type of instrument ISO 13938-2 describes. Product photograph published by a test-equipment seller.

Seams. ISO 13935-1 (strip) and ISO 13935-2 (grab, in a new edition of April 2026) measure the force to rupture a sewn seam pulled at right angles to it. ISO 13936 measures how far the yarns slip at a seam in woven fabric, in three parts: fixed seam opening, fixed load and needle clamp. ASTM’s method is D1683/D1683M, failure in sewn seams of woven fabrics.

Pilling and abrasion standards

Pilling. The four parts of ISO 12945, all in 2020 editions, differ in how the surface is roughened: part 1 tumbles specimens in a rotating pilling box, part 2 rubs them on a modified Martindale tester, and part 3 uses a random tumble pilling tester, which ISO applies to most woven and knitted fabrics including napped fabrics such as fleece. Part 4 sets out the visual assessment of pilling, fuzzing and matting. ASTM’s methods are D3512/D3512M (random tumble), D3511/D3511M (brush) and D4970/D4970M (Martindale). Because the machines work the surface so differently, a pilling grade has to be read with the method and the number of rubs or minutes behind it.

Abrasion. ISO 12947 is the Martindale method in four parts: part 1 the apparatus, part 2 specimen breakdown, found by inspecting the specimen at fixed intervals, part 3 mass loss and part 4 change of appearance. Part 2 applies to all fabrics including nonwovens but not to coated fabrics, for which ISO points to ISO 5470. ASTM has D4966 (Martindale), D4157 (oscillatory cylinder) and D3884, a guide to the rotary platform abrader.

Chemical tests: fibre content, pH and formaldehyde

Fibre identification and content. ISO/TR 11827, a technical report rather than a standard, describes procedures for identifying natural and man-made fibres. AATCC TM20 uses physical, chemical and microscopical techniques to identify fibres, including the generic fibre types defined under the US Textile Fiber Products Identification Act. The blend percentage is then found by quantitative analysis: ISO 1833-1 sets the common method, and most of the other 27 current parts of ISO 1833 dissolve one fibre out of a named mixture, such as part 11 for certain cellulose fibres with certain other fibres using sulfuric acid, or part 20 for elastane mixtures using dimethylacetamide. AATCC TM20A determines moisture, non-fibrous content and fibre composition by mechanical, chemical and microscopical methods. ASTM no longer has a live method for either job: its list shows D276 on fibre identification withdrawn in 2021 and D629 on quantitative analysis withdrawn in 2024. The site’s guide to fibre identification tests covers the burning, microscope and solubility tests in more detail.

pH. ISO 3071 measures the pH of the water extract of textiles in any form, from fibre to fabric. AATCC TM81 does the same for wet-processed textiles, extracting the chemicals that influence pH into water and reading the extract with a pH meter.

Formaldehyde. The methods measure different things, so their results should not be compared directly. ISO 14184-1 extracts free and hydrolysed formaldehyde in water and works between 16 and 3,500 mg/kg; below 16 mg/kg the result is reported as not detectable. ISO 14184-2 measures formaldehyde released into the vapour, and ISO 14184-3 (2023) measures free and hydrolysed formaldehyde by liquid chromatography. AATCC TM112 suspends the fabric over water in a sealed jar under accelerated storage and measures what is released. Limits for restricted substances such as PFAS are set by regulation; see PFAS in textiles: limits, dates and test methods by market.

Conditioning, construction and fabric properties

Conditioning. Fibres take up moisture, and moisture changes weight, strength and dimensions, so physical tests are run on conditioned specimens. ISO 139 defines a standard atmosphere for conditioning and for testing physical and mechanical properties, plus a standard alternative atmosphere that may be used if the parties agree. ASTM D1776/D1776M covers conditioning wherever a test method calls for it, with a preconditioning step because earlier exposure to high or low humidity affects how much moisture the textile takes up.

Fabric weight and construction. ISO 3801 determines mass per unit length and mass per unit area of woven fabrics, on whole pieces or on samples, and ASTM D3776/D3776M does the same for fabric in general. The arithmetic is simple: a 100 cm² disc is one hundredth of a square metre, so a disc weighing 1.52 g comes from a 152 g/m² fabric. ISO 7211-2, revised in 2024, counts threads per centimetre by three methods (dissection, counting glass, traversing thread counter), with dissection deciding any dispute; ASTM D3775 counts ends and picks. To work weight back from ends, picks and yarn count, see weaving calculations; for yarn count systems, yarn spinning formulas.

A floor-standing air permeability tester with a red worktop, a circular test head clamped by a lever arm, and a control box with a display screen
An air permeability tester of the kind used for ISO 9237 and ASTM D737. Product photograph published by a test-equipment seller.

Air, water and oil. ISO 9237 measures the air permeability of most fabrics, including industrial fabrics, nonwovens and made-up articles; ASTM’s method is D737. ISO 4920 and AATCC TM22 are spray tests of resistance to surface wetting; ISO warns that its spray test does not predict rain penetration, because it does not measure water passing through the fabric. That is the job of ISO 811, the hydrostatic pressure test for fabrics meant to resist water. Oil repellency is AATCC TM118 or ISO 14419, and thickness ISO 5084 or ASTM D1777.

Yarn. Yarn count by the skein method is ISO 2060 or ASTM D1907/D1907M, and single-end breaking force and elongation is ISO 2062 or ASTM D2256/D2256M.

Garment testing standards

Garments are tested with the fabric methods above, plus those written for made-up articles: ISO 5077 and AATCC TM150 for the dimensional change of whole garments, and the seam methods ISO 13935, ISO 13936 and ASTM D1683/D1683M. A buyer’s test protocol lists which of them apply and the grade or value each must reach; the site’s page on apparel testing goes through the tests a typical protocol asks for, and choosing a third-party testing laboratory covers who runs them.

Two standards sit around the tests rather than in them. ASTM D5430 grades fabric by visual inspection and may be used, when purchaser and seller agree, to accept individual rolls and shipments; ASTM notes that the penalty points for the same rolls can vary considerably between its point-assignment options, so the same option should be used when the two sides disagree. The four-point defect index calculator does the arithmetic of the four-point system, and the site’s guide to fabric inspection explains the practice. ISO 2859-1, a general standard on sampling by attributes rather than a textile one, sets the AQL sampling plans used to decide how many garments in a lot to inspect; the AQL sampling plan calculator applies it.

Legal safety requirements sit outside the test methods. In the United States, 16 CFR Part 1610, the Standard for the Flammability of Clothing Textiles, sets methods for testing clothing textiles and three classes of flammability, and warns against textiles whose burning is unsuitable for clothing. ISO’s methods for the burning behaviour of fabrics, ISO 6940 (ease of ignition) and ISO 6941 (flame spread), both have 2026 editions.

Where to get the standards, and the PDF question

The full texts are copyright documents sold by their publishers. ISO sells its standards through its own store and its national members; AATCC sells its methods through its store, where AATCC TM61 was priced at US$75 for members and US$100 list on 11 October 2026; ASTM listed D5034 at US$72 the same day. What is free is the catalogue entry: ISO’s page for each standard gives its abstract, edition, stage and committee, AATCC’s store page gives the purpose and scope, and ASTM’s store page gives the scope and significance. China’s standards portal lists GB/T 3921 but does not display its text, explaining that the standard adopts an international one and is protected by copyright. A full text offered free elsewhere is not the publisher’s and may be out of date: the earlier version of this page linked a third-party sample of ASTM D629-15, a method ASTM has since withdrawn. The reference that can be kept and printed is the pair of tables on this page.

Questions

What are the main textile testing standards?

The methods of ISO (ISO/TC 38 Textiles), AATCC and ASTM (Committee D13). Common examples are the ISO 105 colour fastness series, ISO 5077 with ISO 6330 for shrinkage, ISO 13934 for tensile strength, ISO 12945 for pilling, ISO 1833 for fibre content and ISO 139 for conditioning, with AATCC TM61, TM8 and TM135 and ASTM D5034, D3512 and D3776 as their American counterparts.

What are the ISO test methods for textiles?

There is no single ISO textile testing standard. ISO/TC 38 and its subcommittees had 456 published standards on 11 October 2026, a count that includes updates, most of them test methods, from ISO 139 (conditioning atmospheres) to the ISO 105 colour fastness series with its 94 current parts. The table at the top of this page pairs the common ones with their AATCC and ASTM counterparts.

What are AATCC test methods?

The standards of the American Association of Textile Chemists and Colorists, designated TM for test methods, EP for evaluation procedures and LP for laboratory procedures, then a number and a year, such as AATCC TM61-2013e(2020)e2. They concentrate on colour fastness, wet testing and chemical analysis, and are sold through the AATCC store.

What is the difference between ISO 105-C06 and AATCC 61?

Both test colour fastness to laundering, but they are built differently. ISO says one single (S) test of ISO 105-C06 closely approximates one laundering and one multiple (M) test up to five; AATCC says one 45-minute test of TM61 roughly approximates five home launderings. The results are not interchangeable, so a report should name the method and the test condition used.

Which standards are used for garment testing?

The fabric methods above, plus ISO 5077 or AATCC TM150 for the dimensional change of garments, ISO 13935 and ISO 13936 or ASTM D1683/D1683M for seams, ASTM D5430 for inspecting fabric and ISO 2859-1 for sampling a lot. The buyer’s protocol, and laws such as 16 CFR Part 1610 in the United States, set the results the garment must reach.

Is there a free PDF of the ISO textile testing standards?

Not of the full texts, which ISO and its national members sell. ISO’s catalogue page for each standard gives its scope, edition and status free, and the tables on this page are a reference list of the methods, their counterparts and their current editions that can be printed and kept.

Sources

How this page is kept

Last verified 11 October 2026. Every standard number, edition, status and scope line on this page was read that day from the publisher’s own catalogue page: ISO’s catalogue, the AATCC store and ASTM’s committee lists and store. Counts of ISO and ASTM standards are the publishers’ own figures on that date. The worked examples use the site’s calculators as they stood on that date. Editions change at each review, so the latest-versions table is checked against the publishers again whenever this page is revised.

Change log. 11 October 2026: rewritten in full as a reference to which standard covers which test, with the current editions, how the numbers are read, and a worked shrinkage and tensile example. Corrected from the earlier version of this page: ASTM D1686, listed there as a key textile method, is a method of ASTM subcommittee D16.02 for the colour of molten aromatic hydrocarbons, not a textile test; ISO 6330 is a washing and drying procedure, not by itself a dimensional stability test, which is ISO 5077; the earlier page described ASTM as focused on chemical tests, whereas AATCC describes its own methods as the chemical and wet-testing ones and ASTM’s as physical; its “quality score” formula, which added tensile strength, elongation and a colour fastness grade, is not from any standard and has been removed; and its downloadable PDF pointed to a third-party sample of ASTM D629-15, a method ASTM withdrew in 2024.

Found an error? Please tell us through the contact page, naming the section and the source that disagrees.

Leave a Comment

Your email address will not be published. Required fields are marked *

Scroll to Top

Follow on WhatsApp

Scan with your phone’s camera to open the channel, then tap Follow.

QR code for the WhatsApp channelOr open WhatsApp on this device

The Selvedge · free · one email a week

Know what changed in textiles this week.

Our register tracks 3,130 textile standards. Nobody reads them all, so once a week we tell you which ones moved, and what else is new.

  • Standards added, revised or withdrawn that week
  • One textile calculation, worked through to its answer
  • New and revised guides on the site
  • Textile fairs coming up, with their dates

Free when you confirm: Spinning and Weaving Calculations (PDF). 49 calculations, from the blowroom to the loom, each with its formulas and a worked example.

We send a confirmation link first. Unsubscribe in one click, any time.

  • No spam
  • Your address is not shared
  • Unsubscribe in one click